Cast Alnico Magnets 1

Cast AlNiCo Magnets

Alnico magnets are made primarily from aluminum, nickel, cobalt, copper, iron and sometimes titanium. The composition of alnico alloys is typically 8?C12% Al, 15?C26% Ni, 5?C24% Co, up to 6% Cu, up to 1% Ti, and the balance is Fe. They can be either cast or sintered. Cast alnico magnets is melted and and poured into a mold. Once solidified, the material is rough ground and then heat-treated and cooled, sometimes in a magnetic field. When treated in the presence of a magnetic field, the magnet is called anisotropic. This orients the material to take on maximum magnetization and allows a higher gauss level. A cast alnico magnetthat is not heat-treated in a magnetic field is called isotropic. After heat treatment and cooling, the material can be ground to specific tolerances and then magnetized.

Magnetic Properties of Cast AlNiCo Magnets

Grade Remanence
Br
Coercivity Force
Hcb
Max. Energy Product( BH )max max. continuous
temperature
US standard IEC standard
mT kGs kA/m Oe kJ/m3 MGOe
LN10 650 6500 42 530 10 1.2 810 Alnico 3 Alnico 9/3
LNG11 720 7200 37 480 11.2 1.4 810 Alnico 1 Alnico 8/4
LNG13 700 7000 50 620 13 1.6 810 Alnico 2 Alnico 12/6
LNGT18 580 5800 90 1130 18 2.26 860 [I.Alnico 8] Alnico 17/9
LNG16 800 8000 53 660 16 2 850 [Alnico 4] /
LNG34 1180 11800 44 550 35 4.3 860 [Alnico 5C] /
LNG37 1180 11800 48 600 37 4.65 860 [Alnico 5C] Alnico 37/5
LNG40 1220 12200 48 600 40 5 860 Alnico 5 /
LNG44 1220 12200 52 650 44 5.5 860 Alnico 5 Alnico 44/5
LNG52 1250 12500 55 690 52 6.5 860 Alnico 5 DG Alnico 52/6
LNG60 1300 13000 56 700 60 7.5 860 Alnico 5~7 /
LNGT28 1050 10500 56 700 28 3.5 860 Alnico 6 Alnico 26/6
LNGT32 800 8000 104 1300 34 4.25 860 Alnico 8 Alnico 38/11
LNGT38 820 8200 110 1380 38 4.75 860 Alnico 8 Alnico 38/11
LNGT44 880 8800 120 1500 44 5.5 860 Alnico 8 /
LNGT60 900 9000 110 1380 60 7.5 860 Alnico 8 Alnico 60/11
LNGT72 1050 10500 112 1410 72 9 860 Alnico 9 /
LNGT36J 700 7000 140 1750 36 4.5 860 Alnico 8 HC Alnico 36/15